I´m suffering from the exact same thing here. Did you find any solution for your problem @drkhurram? I have to go to printer every two hours to cut the twisted filament and restart the print.
I´m suffering from the exact same thing here. Did you find any solution for your problem @drkhurram? I have to go to printer every two hours to cut the twisted filament and restart the print.
I was planning on getting this material for the S5, as the hardest and strongest material to print, but, Reading this is pushing me back, what are your outcomes to the problem?
Recommended Posts
UlrichC-DE 115
Hello
I do not know these problems with it.
I always take into account that PAHT CF15 absorbs moisture very quickly and a lot.
If you do not print this dry at 10% material moisture, virtually anything can happen.
The material then boils in the nozzle. It also pops now and then and the prints look like tar lumps.
Is your material dried?