Usually as a rule of thumb I use these ratios for PLA (different brands may vary)
0.1 | 25mm/s | 195ºC
0.1 | 50mm/s | 210ºC
0.1 | 80mm/s | 235ºC
If you see some of this stringing occur during the print, in the tune menu you can tweak the settings (increase or decrease temperature) until it disappears.
Eventually you'll develop a pretty good feel for this right away
- 1
Recommended Posts
DidierKlein 729
Hi Frederiek,
To reduce stringing you can:
Reduce the temperature, for you settings 0.06mm layers at 25mm/s i think you can drop it to 200°c or lower. This will reduce oozing.
You can also increase the travel speed to 250mm/s
Did you change anything in the retraction settings on the printer?